Introduction:For welding 0Cr19Ni9 stainless steel structures,which working temperature is below 300°C.
Standard &Typical Chemical Composition of Deposited Metal (%)
Element
|
C
|
Mn
|
Si
|
S
|
P
|
Cu
|
Ni
|
Mo
|
Cr
|
Specification
|
≤0.08
|
0.5-2.5
|
≤0.90
|
≤0.030
|
≤0.030
|
≤0.75
|
9.0-11.0
|
≤0.75
|
18.0-21.0
|
Actual Result
|
0.057
|
1.35
|
0.41
|
0.007
|
0.021
|
0.20
|
9.75
|
0.15
|
19.78
|
Standard & Typical Properties of Deposited Metal
Test Item
|
Tensile Strength Rm (MPa)
|
Elongation A(%)
|
specification
|
≥550
|
≥35
|
Actual Result
|
630
|
42
|
Size and Current (DC+)
Dia.(mm)
|
2.5
|
3.2
|
4.0
|
5.0
|
|
Length(mm)
|
250
|
350
|
350
|
350
|
|
Current(A)
|
F
|
60-80
|
90-110
|
120-160
|
150-200
|
V,OH
|
50-70
|
80-100
|
100-150
|
-
|